Online Quality Monitoring in Laser Welding of Heat Exchangers

More than 200 tube-to-tubesheet laser welds per heat exchanger, made in under four minutes - and each one has to be leak-tight. In 2020 RMA implemented real-time weld monitoring on AIC's VC heat exchanger line, so defects are detected while the weld is being made, not after the pressure test.

The application

AIC S.A., RMA’s parent company, manufactures stainless steel heat exchangers. Depending on the product type, 50-95% of all welded joints at AIC are laser welds, and the factory ships thousands of kilometers of laser seams every year. At that volume, quality control after the fact is not enough.

The test case was the VC family of shell-and-tube heat exchangers. A set of scanner heads makes over 200 tube-to-tubesheet joints in less than 4 minutes:

ParameterValue
Joint typeTube-to-tubesheet (ASME)
TubesØ16 × 1 mm, ferritic stainless steel UNS S43932
Tubesheet1.6 mm, same material
Required penetration1.25-1.5 mm from the weld face
Tube protrusion0.4 ± 0.4 mm above the tubesheet
RequirementsASME Section IV and VIII Div. 1, pressure test 75 PSI
Tube-to-tubesheet joint geometry: tube Ø16 × 1 mm, tubesheet 1.6 mm, penetration 1.25-1.5 mm, protrusion 0.4 ± 0.4 mm
VC exchanger, tubesheet and joint geometry (Rys. = Fig.).

What goes wrong

The most frequent problem is unrepeatable part position after assembly: tubes protruding too far or too little, and a varying gap between tube and tubesheet hole. Occasionally the process itself drifts - laser power drops because of contaminated optics, shielding gas runs short, or the focal position shifts. Each of these can cause insufficient penetration, an uneven weld face or porosity.

The solution: Precitec LWM

After a series of laboratory tests, the RMA team implemented the Precitec Laser Welding Monitor (LWM) in Q3 2020. Sensors in the optical path of the welding head record three signals at once:

  • visible light from the process,
  • laser radiation reflected back from the weld,
  • thermal radiation in the infrared (SWIR).

Each signal has its own curve over the weld time; together they form a fingerprint of a reference weld. A defined defect or deviation shows up immediately in the recorded data, and the system classifies anomalies as weld defects or process faults (such as too little shielding gas or dirty optics).

Defects detected by the online system with the corresponding LWM signal curves: tube protruding by 3 mm, laser power drop of 200 W, welding without shielding gas
Examples detected online, left to right: tube protruding by 3 mm, laser power drop of 200 W, welding without shielding gas.
Tubesheet before welding, welds after welding and welds after laser ablation cleaning
Left to right: tubesheet before welding, welds after welding, welds after laser ablation.

What the project showed

  • Defects are found during production, so deviations are corrected before they turn into scrap or failed pressure tests.
  • Production data links defect type, frequency and position to upstream causes - assembly, part preparation and incoming component quality.
  • Quality records are tied to individual welds, which supports traceability over the product’s service life, warranty and service.

What it shows today

Per-joint monitoring with an auditable log is now a standard stage of RMA’s process control in battery welding - the same principle, applied to cell terminals, tabs and busbars instead of tubes. For heat exchanger applications, see heat exchangers.

DOWNLOAD

Battery Welder Spot

AVAILABLE FROM STOCK

Battery Welder Spot - available now

A Battery Welder Spot is in stock and ready to ship. Contact us for details.

sales@myrma.eu

BROCHURE 2026 - PDF

Download the brochure

Enter your email and the download starts right away.

This form is protected by reCAPTCHA - Google's Privacy Policy and Terms of Service apply.