KNOWLEDGE · APPLICATION NOTE

Laser Welding Heat Exchangers

A heat exchanger has to be leak-tight at every joint, and there can be hundreds of them. We show why laser welding fits the job, using the line we built for AIC as the example: more than 200 tube-to-tubesheet welds in under four minutes, each one checked while it is being welded.

Laser welding has become one of the standard joining methods in heat exchanger production. The reasons are practical: high speed, repeatable welds, little heat going into thin walls, and easy automation. Below we show what that looks like in a real project.

What a heat exchanger asks of a weld

Every joint has to be strong and leak-tight, and thin-walled tubes and tubesheets must not distort or overheat. On top of that, penetration has to be the same across hundreds of joints on one exchanger. A laser gives close control of the weld pool and a narrow heat-affected zone, which matters most on stainless steel and aluminum. Narrow, deep welds and joints close to heat-sensitive parts are typical keyhole-mode work.

Example: the VC heat exchanger line for AIC

AIC S.A., RMA’s parent company, manufactures stainless steel heat exchangers. Depending on the exchanger type, 50-95% of all welded joints at AIC are laser welds, and the factory ships thousands of kilometers of laser seams every year.

For the VC family of shell-and-tube exchangers we built a fully automated line. RMA MLS501 and MLS502 laser welding machines with scanner heads are served by an industrial robot that moves the exchangers between stations. Five machines, three laser sources and the robot are controlled from one panel on the COPA-DATA zenon platform, with recipes for each product type. Details are in the line case study.

Scanner head, camera and fume extraction inside an MLS laser welding machine
Scanner head with camera and fume extraction in an MLS machine.

The tube-to-tubesheet joint

One VC exchanger has more than 200 tube-to-tubesheet joints. The set of scanner heads welds them in under 4 minutes.

ParameterValue
Joint typetube-to-tubesheet (ASME)
TubesØ16 × 1 mm, ferritic stainless steel UNS S43932
Tubesheet1.6 mm, same material
Required penetration1.25-1.5 mm from the weld face
Tube protrusion0.4 ± 0.4 mm above the tubesheet
RequirementsASME Section IV and VIII Div. 1, pressure test 75 PSI
Tube-to-tubesheet joint geometry: tube Ø16 × 1 mm, tubesheet 1.6 mm, penetration 1.25-1.5 mm, protrusion 0.4 ± 0.4 mm
VC exchanger, tubesheet and joint geometry (Rys. = Fig.).

What can go wrong

The most common problem is not the laser but assembly. Tubes protrude too far or not far enough, and the gap between tube and tubesheet hole varies. Less often the process drifts: power drops because of dirty optics, shielding gas runs short, or the focus shifts. Any of these can mean too little penetration, an uneven weld face or porosity. With 200 welds per part, visual inspection alone will not catch it.

Monitoring every weld

In 2020 we installed the Precitec Laser Welding Monitor (LWM) on this line. Sensors in the optical path of the head record visible process light, reflected laser radiation and infrared thermal radiation at the same time. Together they form the reference curve of a good weld. When a weld deviates from it, the system shows it and tells a weld defect apart from a process problem such as too little gas or dirty optics. Defects are caught during production, not at the pressure test. More in the online monitoring case study.

Defects detected by the online system with the corresponding LWM signal curves: tube protruding by 3 mm, laser power drop of 200 W, welding without shielding gas
Examples detected online, left to right: tube protruding by 3 mm, laser power drop of 200 W, welding without shielding gas.

On this line the welds also go through laser ablation. The images below show the same area of the tubesheet at three stages.

Tubesheet before welding, welds after welding and welds after laser ablation cleaning
Left to right: tubesheet before welding, welds after welding, welds after laser ablation.

Data for every weld

Monitoring records are tied to individual welds. On the VC project that gave two things. First, traceability over the whole service life, warranty and maintenance of the exchanger. Second, a way to link the type, frequency and location of defects to causes earlier in the chain: assembly, part preparation and component quality. We apply the same principle today in the control architecture of every RMA machine.

Not everything has to be laser welded

We have also built heat exchanger lines where the laser is not the main process. The tube bundle production line with five KUKA robots changes over by itself, expands the tubes, trims them to 0.1 mm and orbitally welds them to the tubesheets. On the economizer production line two robots TIG weld the product, and an RMA-designed system changes the electrodes. We choose the process to fit the joint and the product, not the other way round.

Heat exchangers at RMA

Projects for heat exchanger manufacturers start with trials on real parts in the Laser Application Center. We check penetration, assembly tolerances and the quality-control method before we design the machine. More about the industry: heat exchangers.

FREQUENTLY ASKED QUESTIONS

Why does laser welding suit heat exchangers?

The laser puts little heat into the part, so thin-walled tubes and tubesheets distort less and the narrow heat-affected zone protects stainless steel. The process is also fast, repeatable and easy to automate, which matters when one exchanger has hundreds of joints.

How many laser welds does one heat exchanger have?

It depends on the design. AIC's VC shell-and-tube exchangers have more than 200 tube-to-tubesheet joints, which the RMA line welds in under 4 minutes. At AIC, laser welds make up 50-95% of all welded joints, depending on the exchanger type.

How is weld quality checked during production?

A monitoring system in the welding head records process light, reflected laser radiation and thermal radiation. Each weld has its own signal curve, compared with a reference, so insufficient penetration, missing shielding gas or a power drop show up immediately instead of at the pressure test.

Is laser welding always the right choice for heat exchangers?

Not always. On the economizer production line RMA used robotic TIG welding because it suited that product best. The process is chosen for the joint, the material and the customer's requirements.